I. Calculation of Paint Consumption for Steel Structures
The calculation of paint consumption for steel structures involves three steps: calculating the area → determining the theoretical consumption → multiplying by the loss factor.
1. Calculate the surface area of the steel structure
? Lookup method: For standard components such as H-beams and steel pipes, refer to the "Theoretical Weight Table of Steel" to obtain the "cross-sectional area per meter" and multiply it by the length.
? Experience value: For general steel structures, it can be estimated at 25–30 m2/ton; for light steel (such as purlins), approximately 32 m2/ton, and for heavy steel, about 14 m2/ton.
? Formula Method (Steel Plate): Area (m2) = Weight (kg) ÷ [7.85 × Thickness (m)].
2. Calculate the theoretical dosage (no loss)
Core parameters: Volume solids content (VS%, refer to the paint instruction manual), Design dry film thickness (DFT, μm).
In liters (L):
? Theoretical Coating Rate = (VS × 10) ÷ DFT (m2/L)
? Theoretical usage = Area ÷ Theoretical coverage rate (L)
In kilograms (kg):
? Theoretical dosage (kg) = Area × DFT ÷ (VS × 10) × Density (kg/L)
Calculation example: Area 1200 m2, VS = 65%, DFT = 80 μm, density = 1.4 kg/L.
Theoretical coating rate = 65 × 10 ÷ 80 = 8.125 m2/L
Theoretical dosage = 1200 ÷ 8.125 ≈ 148 L (or 148 × 1.4 ≈ 207 kg)
3. Calculate the actual procurement quantity (including losses)
Actual quantity = Theoretical quantity × Loss factor. The comprehensive loss factor for steel structures is generally set at 1.5 to 2.5, with a common budgetary value of 1.8.
Reference values for loss coefficients of different construction methods:
Construction Method Reference Range of Loss Coefficient
Airless Spray 1.5 ~ 1.8
Air spray 1.8 ~ 2.0
Brushing / Roller coating 1.1 ~ 1.3
Complex structures (utility tunnels, multi-node systems) 2.0 ~ 2.5
Additional note: If the theoretical coating rate corresponding to a known dry film thickness (e.g., 80 μm) is known, the value must be converted when the actual dry film thickness changes
? Corrected coating rate = Original coating rate × Original dry film thickness ÷ Actual dry film thickness
II、 Analysis of Paint Loss in Steel Structures
Dry film thickness=construction area ÷ actual coating rate=construction area × CF ÷ theoretical coating rate=theoretical usage × CF, where CF is the loss coefficient.
The loss coefficient CF mainly consists of the following four parts:
1. Loss caused by surface roughness of the workpiece
When painting the surface after spray treatment, the film thickness at the peak of the steel plate is smaller than that at the valley. In order to meet the anti-corrosion thickness requirements at the peak (to avoid pitting), the paint hidden in the trough and pit cannot be included in the effective film thickness, forming a "steel plate roughness consumption loss".
2. Loss caused by uneven distribution of paint film thickness
When inspecting the paint film after construction, the technical service representative, supervisor, or owner will sign off as qualified for areas where the film thickness reaches or exceeds the specified value; The part that does not reach the specified film thickness is required to be repainted, which will inevitably cause "excessive thickness" loss. The main factors causing uneven distribution of paint film thickness are:
? Worker proficiency level;
? Construction environment;
Construction workpieces are simple (flat workpieces) or complex;
Construction methods (airless spraying, air spraying, brush coating, roller coating).
3. Construction waste
The waste of paint that does not adhere to the surface of the workpiece and is lost to the surrounding environment or ground. The typical loss rates of different methods are as follows:
Construction method loss rate
Airless spraying about 10% to 20%
Air spraying with over 50% coverage
Roll coating about 5%
If the brushing control is appropriate, it will be relatively less
Strong wind environment (such as bridge painting) can cause over 100% damage
4. Waste of residual paint in containers
After the construction is completed, the average loss of paint remaining on the inner wall of the paint bucket and in the paint delivery pipe (such as rubber hose) is about 5%.
In summary, the paint loss coefficient during construction is mainly caused by four parts: surface roughness loss of the workpiece, uneven distribution of paint film thickness loss, construction waste, and residual paint waste in the container.
III、 Acceptance criteria for dry film thickness
When the completion acceptance of heavy-duty anti-corrosion coating is completed, the "90-10 film thickness acceptance standard" is often used, which means that the film thickness values measured at more than 90% of the measuring points must reach or exceed the specified film thickness value, and the film thickness values measured at the remaining less than 10% of the measuring points must not be lower than 90% of the specified film thickness index. The selection of measuring points should be representative, and the total area of the tested area should be greater than or equal to 5% of the total coating area.
Example of acceptance steps
Condition: The total area of the heavy-duty anti-corrosion coating is 3200 m 2, and the specified coating thickness is 200 μ m.
Step 1: Determine the sampling area
Choose any 16 areas, each with an area of 10 m 2, and each individual 10 m 2 area cannot be disconnected. Select a total area of 160 m 2, which is exactly 5% of the total area (3200 × 0.05=160 m 2).
Step 2: Layout and Measurement
Randomly determine 5 squares with an area of 50 cm 2 in each 10 m 2 area, and select 3 points within each square for measurement. The film thickness of each square is taken as the average of its three readings, and a total of 80 data points can be obtained in this example (5 × 16=80).
Step 3: Judgment Rules
Out of 80 data points, 10% (i.e. 8) can be allowed to be below 200 μ m, but each individual film thickness reading must not be lower than 90% of the standard film thickness index, which is not lower than 180 μ m.