NEWS AND INFORMATION

首页 > 媒体中心 > Why Weld Access Holes Are Inevitable

Home > Media center >

Why Weld Access Holes Are Inevitable

Time: 2026-11-04 00:00:00

TECH DEPT · STEEL WELDING

Why Weld Access Holes Are Inevitable
A mechanical necessity, not "cutting corners"

The small hole often mistaken for poor workmanship, and why it must exist

From fabrication principles and three mechanical reasons to dimensions, sequence and code comparison, GB 50661-2011 and AWS D1.1 explained in one read.

GB 50661-2011AWS D1.1Welding

01 Basic Concept of Weld Access Holes

A weld access hole (also called a weld pass-through hole, or "rat hole") is a deliberate fabrication opening reserved at the junction of a secondary member and a primary weld in steel structure fabrication. It serves three core purposes: to make room for the welding gun and backing, to ensure the primary weld is deposited continuously and completely, and to avoid the stress concentration caused by densely intersecting orthogonal welds.

The most typical case is the rigid connection of an H-shaped beam to a column (or end plate): the beam's top and bottom flanges must be welded to the column flange by complete-penetration groove welds. If the web end bears directly against the column face, the web will shield the gun, creating an unreachable dead zone at the flange root near the web. An arc-shaped (fan-shaped) cutout is therefore opened at the web end so the gun can reach and complete the weld, and that cutout is the weld access hole.

Main Functions

■  Ensure weld quality: the primary weld (e.g., flange butt weld) can be made continuously, avoiding lack of penetration, slag inclusion, and lack of fusion.

■  Reduce stress concentration: avoids forming a triaxial orthogonal weld field, lowers the peak residual stress, and improves the fatigue and seismic performance of the joint.

■  Ensure weld accessibility: provides working space and a passage for the welding gun, backing, and runoff tabs.

Basic Construction Requirements

■  Curved transition at edges: sharp right angles or corners are strictly forbidden, as fatigue cracks readily initiate at such corners.

■  No weld filling: codes generally forbid sealing the access hole by build-up welding; where appearance or corrosion protection demands it, an adhesive material may be used to close it.

CODE BASIS

The current GB 50661-2011, Clause 5.7.6, is the principal technical basis for access holes in China; its explanatory notes also give the mechanical rationale behind the requirement.

02 Three Mechanical Reasons

Reason 1: The primary weld must be continuous and cannot be interrupted by a secondary weld

When the web end bears directly against the column flange, the web-end weld intersects head-on with the complete-penetration groove weld between beam and column flanges, forming a cross. As the weld cools and shrinks it is constrained by the surrounding metal, leaving residual tensile stress in and near the weld; when two welds intersect orthogonally at the same location, the shrinkage tensile stresses from both directions superpose in the same local region. Removing the web end to form an access hole lets the primary weld pass through intact and continuous, reducing the restraint at the junction. The GB 50661 commentary puts it this way: the dimensions of the access hole must meet requirements and avoid dense welds in the orthogonal direction, so as to release the shrinkage stress of the weld.

Reason 2: The real danger is the triaxial tensile stress state

From a fracture-mechanics viewpoint, triaxial tensile stress strongly limits the material's capacity for plastic deformation. Once a local defect exists, brittle initiation is highly likely. The superposed shrinkage stress at an orthogonal cross, if it further develops into tension in three directions at once, deprives that local metal of the ability to relax stress through plastic deformation, and it can only release energy by cracking. Worse, this location is often also the crater (arc-termination) end of a weld: every welder knows the crater is prone to craters, slag inclusion, and cracks. The triaxial stress superposition places the most fragile defect precisely at the least favorable point of loading.

Reason 3: Working space must be reserved for the gun and runoff tabs

The access hole is not only to make way for the weld. The complete-penetration groove weld on the beam flange requires the gun to reach the root to achieve full penetration, and after welding a place must be left for the runoff tab, all of which takes space. If the hole is too small, the primary weld cannot be fully penetrated or filled at the pass-through, and lack of fusion and slag inclusion follow; the access hole then becomes useless.

03 Dimensions, Shape and Sequence

3.1 Dimensions: clarifying the two "1.5x"

AWS D1.1 sets explicit geometry requirements for access holes: the length of the hole, measured from the weld toe, shall be not less than 1.5 times the thickness of the pierced material; the height of the hole must be enough to deposit sound weld metal on the adjacent plate and to leave room for the runoff tab, shall not be less than the thickness of the pierced material, and is typically not less than 3/4 in (about 19~20 mm).

GB 50661-2011, Clause 5.7.6(2) stipulates: at the bottom flange the web access-hole height shall equal the web thickness and shall not be less than 20 mm; the distance from the access-hole edge to its intersection with the bottom flange plate, to the fusion line of the column-to-beam flange weld, shall be greater than 10 mm.

A special clarification is needed: the "1.5x" in the AWS text constrains the length along the beam direction; whereas the GB provision related to "1.5x the web thickness" should be understood together with the termination distance of a 1.5x weld size (leg), the two are not the same geometric quantity and must not be confused when cited.

3.2 Shape: the transition must be smooth

Hole edges should adopt a smooth transition; the fillet radius should preferably be not less than the greater of 25 mm or 2x the plate thickness; the hole shape should let the material transition gently toward the adjacent surface, and this must be strictly followed where dynamic loading dominates; the hole-end surface should be welded around and kept free of notches. The mechanical logic is plain: the access hole removes an old stress-concentration point and must itself never become a new one.

3.3 Sequence: weld first, then cut; thick plates need preheat and inspection

GB 50661-2011, Clause 5.7.6(1) provides: the access hole in the web should be formed after the web-to-flange longitudinal weld is completed, together with removal of the run-on and runoff tabs, and the access hole must have a smooth transition. Clause (3) further requires: when the web thickness exceeds 40 mm, thermal cutting of the access hole should be preheated above 65 degree C, and if necessary the cut surface may be ground smooth and then inspected by magnetic particle or penetrant testing.

04 Two Untouchable Red Lines

4.1 No encircling weld or corner-returning

GB 50661-2011, Clause 5.7.6(2) is explicit: the web-to-flange longitudinal weld shall not be routed around the web thickness at the access hole by encircling welding; AWS D1.1 also forbids a fillet weld passing through the access hole to return the corner. "Corner-returning" amounts to re-welding two already-separated welds back into one at the hole end, and all the effort spent releasing the triaxial stress is then wasted.

4.2 No weld filling or sealing

GB 50661-2011, Clause 5.7.6(4): access holes shall not be sealed by build-up welding; where appearance or corrosion protection demands it, an adhesive material may be used to close them. Weld filling defeats all three functions of the access hole and in essence buys a new crack risk with real money.

One more requirement, not a "prohibition" but equally important: the access-hole outline must not be cut arbitrarily on site; it must be built strictly to the drawing.

05 Code Comparison Table
Item GB 50661-2011 Clause 5.7.6 AWS D1.1
Bottom-flange hole height Equals web thickness, and >=20 mm >= pierced-material thickness, typically >=3/4 in (about 19~20 mm)
Length measurement Terminates at 1.5x weld size per drawing >=1.5x pierced-material thickness from weld toe
Fusion-line spacing >10 mm to column-to-beam flange weld fusion line N/A
Fillet radius Smooth transition Not less than 3/8 in (about 10 mm)
Encircling weld Longitudinal weld shall not route around web Fillet weld shall not pass through hole to return corner
Sealing No build-up welding N/A
Thick-plate preheat Web >40 mm preheat >=65 degree C Preheat before thermal cutting; heavy plates grind + MT/PT
06 Conclusion

To the designer, the access hole is a classic detail of "trading local weakening for global safety": the primary weld is continuous, shrinkage stress no longer superposes, and the welder gains room to strike the arc. Yet none of its dimensions (height per web thickness, 10 mm spacing), shape (large radius, no notch), or sequence (cut after welding, preheat and inspect thick plates) can be omitted. Saving a little fabrication cost at the expense of joint safety is a thoroughly disproportionate trade.

To the welder, the drawing's demands, "go around the hole, don't return the corner, don't seal it," are not vexatious obstacles but process experience born of seismic lessons. A tiny hole, leveraging a great weight.

CLOSING

An access hole is not a defect; it is the "escape route" a designer leaves for the structure. Dimensions, shape, sequence, not one may be skipped.